NW'1 7 TH E DENTAL C os m os. VOL . LIII. MARCH 1911 . No. 3 . ORIGINAL COMMUNICATIONS . THE LAWS DETERMINING THE BEHAVIOR OF GOLD IN FUSING AND CASTING . By WESTON A. PRICE, D .D .S ., Oleveland, Ohio . (Read before Section I of the National Dental Association, at its annual meeting, Denver, July 20, 1910 . ) ELDOM if ever, in the history of S the progress of dentistry, has so much confusion and uncertainty ac- underlying these processes, the physical conditions and procedures in detail that are made use of in the various methods companied both the practical results of of manipulating the gold, for they estab- an important mode of procedure, and the lish the fixed conditions with which we interpretation of the processes involved, have to deal . These are as follows : as .has attended the operations involving the fusing and casting of gold, and par- (1) The fusing of gold or an alloy ticularly the cast gold inlay . This confu- of gold directly on to a higher-fusing sion has been occasioned by the fact that metal, as in soldering a bridge with and the fundamental physical properties, first, without an investing medium . of the gold itself, and second, of the ac- (2) Taking an impression of a cavity cessories to its use, were not known to or other surface in thin platinum foil, any branch of science ; and the existing and fusing gold directly into it . troublesome errors and the confusion at- (3) Making a pattern of wax in the tending their interpretation cannot be cavity and removing it and investing in corrected until these physical properties some refractory material, and then, after are known, and the laws under which burning out the wax, casting the gold they operate are heeded . directly into that cavity in the invest- ment . THE VARIOUS METHODS OF MANIPULA- (4) Making an impression of the TING GOLD OR ITS ALLOYS IN CASTING . tooth cavity and surface beyond the cav- ity, and making a model in this of a It will be necessary for us to have very material which is refractory enough and clearly in mind, while studying the laws strong enough to cast directly on, after VOL. LII 1 -19 265 266 THE DENTAL COSMOS . waxing up the cavity in the model, and (8) Action of the molten gold on the investing the model and wax in_ a plaster investing medium . and silica investment material . (9) Change in the dimensions of the (5) Making an impression of the gold with its change of state from liquid tooth cavity and surfaces beyond the cav- to solid. ity as in the last method, then making a (10) Change in the dimensions of the model of fusible metal or amalgam or sul- cooling g9ld . fur, into which the gold cannot be cast (11) Distortion of the mold in the in- directly, then making a wax pattern in vesting medium by the cooling gold . that model, which is removed and in- (12) Stretching of the gold if held vested as in the third method, and the when cooling. casting made into the investment . While all of these variable factors are, essential contributors, to a larger or FACTORS OF ERROR . smaller extent, to the final ; error, none plays so important or `large a part in the Some of the confusing and con fl icting average technique as the change in the effects are as follows : dimensions of the cooling of gold ; and First and chiefest is the decreased size all efforts to determine the extent of of the gold reproduction due to its Own error caused by the cooling gold, when contraction. any or all of these other variable factors Second : It may be distorted, or un- are present, have apparently been not evenlydecreased or increased in size . only unsuccessful, but extremely mislead- Third : It may have a depression or ing, for the results have been the sum hole in its surface . total of all the involved errors . Fourth : It may seem to be enlarged . Fifth : It ma.y be distorted or out of FACTORS OF ERROR IN THE TAGGART proportion. DIRECT METHOD . These conditions have been caused by To illustrate, let us follow seriatim the changes occurring in the materials in- steps of the Taggart direct method tech- volved in the procedure, and the methods nique . The wax for its pattern is put of using them . in the cavity at its workable temperature, The variable factors that have a part which will be for the various inlay waxes in producing these possible errors are- ~ from 95° to 130° F . It is cooled in (1) Change in the dimensions of th e the cavity, to render it firm and strong, impression or the pattern by the cooling to about 67° F ., and. in so doing it con- when removing . tracts, according to its formula, one or (2) Change in the dimensions of this ll` two per cent . of its lineal dimension. If impression or pattern material by change, invested at this temperature an error of in temperature when investing . this definite amount is already carried (3) Change in the shape of the pat= forward, to appear in the final inlay, tern due to the elasticity of the wax . unless it be corrected by some other step . (4) Change in the dimensions of this, If the wax of the pattern, when being investing medium in its process of sety formed and cooled, surrounds the tooth ting . structure, covering outside dimensions, it (5) Change in dimensions of this in~ 'will' be stretched as it cools, and it would vesting medium in the process of heat~,, : by so stretching apparently correct part ing, or heating and cooling . or all of the error of contraction from (6) Effects of the wax or pattern mi , cooling ; but all waxes have elasticity and terial on the investing medium . hence do not remain stretched, which (7) Change in the investment dimef introduces a new uneertainty or error to sions from the pressure of the gold wh change the accumulated error . When the casting. wax pattern is invested, its temperature PRICE .-THE BEHAVIOR OF GOLD IN FUSING AND CASTING . 26 7 will determine partly its dimension, for on heating from 67 ° F . to 100 ° or to BEHAVIOR OF THE INDIVIDUAL MATE- 130° F ., the wax will be expanded, and RIALS USED IN CASTING . if not carried to'the softening point at To work intelligently we must there- which surface tension will distort it or fore know the behavior of the materials where the investment will change its used for each step, and make the un- shape, part or all of the accumulated fixed or variable changes correct the fixed error due to contraction of the wax may changes . The great fixed change is the be corrected, and with a certain definite contraction of the gold both as it changes technique to be explained later, even an its state and as it cools to normal tem- error of expansion produced . The ordi- perature, and these changes will have the nary technique will not show the true largest consideration in this paper, but expansion . . Heating the pattern to en- the other factors are essentials, and must large it will release its elasticity and also be definitely established for the fix- allow much distortion . ing of fundamental rules of procedure . In the next step, of heating the in- We will take them up in sufficient detail vestment material, if it be of the best in the order of their occurrence in the quality we may have an expansion of technique of procedure . about one per cent ., or if of poor qual- The making of relatively exact deter- ity we may have a contraction of two minations requires instruments of very per cent., according to our manipulation, great precision . The writer has had sev- and if the investing compound is soft eral constructed especially for this re- and yielding it can be distorted easily search work, and has had very great by the pressure of the gold when casting, assistance from Prof . Dayton C . Miller, thus causing an error which is not a professor of physics in the Case School uniform expansion . of Applied Science, whose services he When the molten gold is forced into was fortunately able to engage with the the investment,_ its physical state changes use of, very special instruments of pre- from liquid to solid, and here we have cision for the most complicated of these what has heretofore been an entirely un- determinations . known factor, but which we will show later to be a very large contraction ; and FACTORS OF ERROR INVOLVED IN THE again, on changing temperature from its IMPRESSION OR PATTERN MATERIALS freezing-point and cooling to normal tem- (WAXES) . perature, it contracts, as the writer has previously shown, over two per cent . We will study the materials and uses (Items of Interest, May 1908 .) This in their order of sequence . First : The contraction can be partially controlled by change in the dimensions of the impres- pressure on the congealing gold, thus sion or pattern material by cooling when forcing gold from the sprue, and par- being removed from the cavity. Prac- tially by holding the gold as it contracts, tically all the kinds of impression or pat- i .e . by causing it to surround a strong tern material used for inlay work for form, thus preventing the normal con- carving in the cavity have about the same traction . qualities, and the working range in tem- The relation of the size of this final perature varies according to the base used casting of gold to the original cavity in in largest proportion in their manufac- which the wax pattern was made may ture . thus vary through a wide range, and the The carving waxes are not best adapted final error is the sum of all the plus and for taking impressions for any of the minus changes made in the size of the model methods . The following waxes record of the cavity, as it passed through purchased in the open market, and the the different materials and processes . base waxes chiefly used in them, have We will show definitely the amount of been carefully tested for their expansion change produced by each step . co-efficient, working range, and total ex- 268 THE DENTAL COSMOS . pansion from 67° F ., room temperature, method was by measuring the density of to their maximum working temperature : the waxes at various temperatures, which Bird & Moyer, Cleveland Dental, glewe's, gives the volume expansion . The linear Consolidated, Peck's, Price's for Stone expansion is one-third the cubical ex- Model Method, S . S . White black, S . S . pansion . Fig . 2 shows the small bal- White Crown Sticky-wax, Standard, and ance arranged for these determinations . beeswax, gum damar, paraffin, stearic The weight of the wax was measured, acid, bayberry, canawba, and cerecin . while suspended in the beaker of water, The rate of expansion of all waxes at different temperatures. Table I FIG . 1 . ~t . ♦ ~~ Microscope comparator arranged for measuring expansion of wax . changes rapidly with increase of temper- gives the linear expansion, in thou- ature, but at different rates for different sandths of an inch, and the density at base waxes and different formuloe or mix- various temperatures Centigrade of the tures . This made it necessary to deter- various waxes . Table II gives the work- mine very close steps for all the waxes . ing ranges of the various waxes and the This was done by two methods, one by changes in their dimensions, in thou- measuring the expansion directly with sandths of an inch, with changes of a microscope comparator (shown in Fig . temperature Fahrenheit . This table is 1) . The wax bar is heated in a water- a very valuable one, inasmuch as it gives bath and the distance between the pilot the key to much of our error . The lower points or hair lines that are placed on or minimum working range of tempera- the wax bar is measured by micrometer ture of the various waxes can be modified screws, these carrying two microscopes slightly by working the wax. The maxi - which are focused on them . The other mumtemperature is usually higher than PRICE .-THE BEHAVIOR OF GOLD IN FUSING AND CASTING . 26 9 that at which a frail pattern of wax dimensions, or 1 .2 per cent ., which will could be handled and keep its shape, be the error carried forward if it be in- though a block of it could . In Table II vested at this temperature . If, however, the inlay waxes of the market are ar- it be heated at the time of investing, and ranged alphabetically . It also shows the placed in an investment at 130° F., its elasticity when a bar of wax is bent on e maximum working temperature, it wil l FIG. 2 . ; •r ~.~.~ . .W _ . . ... ... . . . l} + i ~'.Stij ..... ... .. S`. . ..' ~~~,^.,,, . • . ww .- - '® .,~ti . . . . ° .. ~ ; .1 . .~ Small balance arranged for measuring density of wax and gold . inch, also one-half inch, at its lower work- expand 36/1000, or 3 .6 per cent . The ing range, and chilled, then heated to latter dimension is 24/1000, or 2 .4 per the upper working range, when it will cent ., larger than when the impression return nearlv to its former position . If wax was in the cavity . And so the be- a wax, say the first one, be placed in a havior of all other waxes is indicated . cavity at its minimum working tempera- This would seem to be a means for cor- ture, 107 ° F ., and cooled down to 67 ° recting, by compensation, all of our diffi- F ., it will contract 12/1000 of its linear culties due to the contraction of the gold, 270 THE DENTAL COSMOS . M 00 GO O " 00 CyO ° • • • • • q O vi ao V N E•, = y . • • . • . . a N M M M V Q ~/Oi . . . . •. . . . . • ~ . o h vJ ~ m u'i in, cd . ~ . . . . . O O~ M a ~O OC u! . . . . . . M M M . . . ~ . w v; GO v) O O M O V) • • O O M Q n ti ~ N N ° M . O Op N ~O 00 v O~ l~ N O~ R O •~-~ M M M d' d~- vMi U~ . . •. T OD l~ ~' OD N O~ W~~l~ O6 00~ . cd~y O G O p ~ Q . '.a . 00 Q W .-~ •-~ .r M T M M O O~ ~ .:.. ol . . . N O N Q n ° N Rf .. .ti •-~ ~ N . N m ,d Ei rn - p , . • 1,I d O tr 10 O u] a0 O: 00 l~ . . • ~V h V N N M _M _ w ~ GV . r/1 O~ y 00 ..• ~ U . ~ O O: •. •. . .. . . W o .. N Q co ~ • ~ p y q >, •i.' vr cn m o .+ rn a ° .v, u • . . . ~ . 0 ~ ~ ~ cl~ m e ~ r n 4 sr . ~ h ~n _ . . . ~ . . . .. . Is O M- ~O 00 M RT •-N-i N ° M . . . . ~ . rz Iq d' . v] h ~O N pM ' ~ • . • ~ A •~ E z •hl .~i .y N M R d' . . . . . . a.~+ O ~•„- .~ N ~ U .• . : . •. ~ • C' O M ~O ~O ~p rl ~O F 00 C/~ I-I /y ~ 11; . c~' 11; 06 y •~-~ N . M . M . . . . . z •N ~ . F 47 ~ ^ 0~ ~ O N O ~ Q ° ~ • • • • . •. M . . . •~ ~T N .O ~.~ b ~y ~ 01 ~ 3+ ~O 1~ m ~p •+ ~Q O I h .U Q . • • . • L~ F .,0 N q I N M M O ~/J Q ~/J . . . ~ ~ . . . _ . . . w ~ ~. . ~ n . ~ ~ ~ . . . . . vi ,A o co o ~ m N . . . .. . . ~ ~ m N a ~ E . . . .i 0 o rn .~ • -. w ~ o ~ • : . ~ p,~ '.d. -r ~n o . . . ~ ++ ~ r~ 0 09 W II O ~O O ~ ~O O~ o N • ~ • • ~ q 4C A .a . . . . a> ..U ... e~ o ~ q 01 7 U •~ F C"l ~ "' O~ O M V' N U ~ . . . . . ~ y O Q O ~ ~~~q q .-i M N RM . • . . . . y~ U A CQ U . . . . . . . ?/ ~ ~ q ~ W ~ O M h o0 wo O . F ~ ~ ed .° . . . . .. . ~ •U n • ~ O . .. ~ H m ❑ q F . . ~ N ~ oo M . . .~ M . n. ~ o~~ . o . • : . . : . . . .~ . . . . . ,. E PRICE .-THE BEI3AVIOR OF GOLD IN FUSING AND CASTING . 27 1 z p • . . . . , F R ~ .. . .. . . .. .. .. ~ z a a U V V W c. O N O O O O O O O • • • C4 pq "Z eD CO ~J uJ .y X0 fJ • . • . z x G' E . . . . . . . . ~.'~. G W q _ . . .. .. .. ,. '. o . . . . . . . . o z c~i A " O q .. . - . . . . . . . . . . . . . . . fJ xp ~ xp f'J ~ 1~- CV ~ O ~ ~'cN M c0 M co dH UO llJ O t_ . . GV . . . . . D4 L1 A a~ O ."~-+ r GV GV C7 . ~ y ^ U M p p d N U . ~' ~ a E o N 8 !M M cD co o C •C~ GO ~o cq O i~ P4 Gq 49 - - r+ N GV • • . . • . • w a z q F H PA xo . . . . C m ai . eD k[J O C O C V. CV m Q O q , ~. CvJ C/J CV GV aV o'J Co ' • GV • • • . k. C U ~ o o a an a _ ~eo F '. , . . . . . . I c cd 'A o ~ co x. ao CO r O o ~ co i i z Ca 0 3 co Co 4V N co Gci V PT4 o z e z a x CO H W E" p~ °~~' 4V Cl GV W d~ cD M O rl ~ . • O . • • • • ti . . . . ~ w to • cq ,-y .y O • 6 s7 A Ck, . . . . . q m :7 cq G] u° eM co M O ~ ~J O cq .ti ,ti • . ,y . . . . . q o 0 0 0 0 0 0 0 0 0 0o 0 o O o 0 CL G+ O C O m cq M O~ ~D ~fJ O C O N O O ~ GV " 6 M cq M M G~7 .r GV GV co Co eD cq4 A uJ O GV co ~ ~• o 0 0 0 0 0 0 0 0 0 o ' . ~ p ° , ~ N 00 ~ :O O d~ ^ .. O Z .. .. . . . . . . . . 3 ~ . ~ q • ~ U . . . . . . . . . . . . y . . . . . . . . . . . c . . . . . . . . . . ~ . z . . . . . . . . w a y g ~ . g ~ . . . . . . . . . z • ~ o .°3 ,.d •q w° "~ . y 3 '-~ ~ ~ A q i t U r~, U P. P: v1 B v~ .~l m 0 C3 Qz, P-i 65 U U p 272 THE DENTAL COSMOS. 9 rn ~ l t ~ ~ ^~ t h t OT N 1 tl ~ v ~ c ~ 10 o ~ ~ n t ` JLL_! co t FA `` V 1 0 0 'Et~ 1 \ ~ ~\ \ z 0 ` `\ \1 .. '\ co 0 `, ~t \ \ t 0 \ t \ \ \ 1 M - \ \ ( , 1 O rn , 11 0 M a; tJ ~ n °4-3 ~ ~ (t\ t , ~ °a \ 1 ~ d \ 1 ~t Ga d d ~ m o cs Q o N a m ~ •qoat as ;o s1Z4Passnoql ul `aotsnudxa aeaul7 { { PRICE .-THE BEHAVIOR OF GOLD IN FUSING AND CASTING . 27 3 but it does not, as will presently be when treated in the same way, straighten shown . Fig . 3 shows diagrammatically 79 per cent . of the distance of the second the exact expansion of all the different bending . The brittle carving waxes are waxes from 67° F ., or its equivalent 20° Peck's, S . S . White, Bird & Moyer, C., to any temperature up to the limit of Standard, and Consolidated, and all these its working range . It also shows graph- have a large elasticity. When a stick of ically the relative behavior of all the each, three inches long, is bent one-half different waxes tested . The base line, inch from straight, held while cooling reading from left to right, indicates the and then released, it will straighten progressive increase from 67° in temper- again, usually about half way to straight, ature in units Fahrenheit, and the top but this differs with the different waxes the corresponding temperature in units and temperatures when bent . The last Centigrade from 20° . The elevation of colLmin of Table II shows the amount, the curve as shown by the figures on the expressed in percentage, of the elasticity left side reads the linear expansion, in or return of wax bars bent both one-half thousandths, of its dimension, or can inch and either one or two inches, as be read in hundredths, as per cent ., they would stand-for the brittle carv- by leaving off the second cipher . From ing waxes would break before bending this chart can be seen at a glance the two inches . exact change in dimension of any of the The error that is possible from this waxes between any two temperatures be- source is enormous, and it will always tween 67 ° F ., and its working limit . All be a distortion, not a uniform expansion waxes are taken as zero dimension at or contraction, therefore it cannot be 67° F ., or 20° C ., temperature . It will corrected by another step . For example, be noted how the increase in the rate of see Fig. 4, A and B . If two wax bars of expansion with the increase of tempera- Cleveland dental inlay wax, or of almost ture is shown by the lines deflecting up- any wax on the market, are heated to the ward more rapidly as the temperature lower working range, one being pulled or increases . These determinations are stretched while chilling and the other made on samples of cast wax, to avoid pushed endwise or compressed (both just the errors of elasticity which form the as the wax could be in a cavity) each then most treacherous error we have to con- being chilled while held, and then carved tend with, and which I fear that few to be identical, they represent the same have either suspected or recognized . If size and form, in this case one inch in you will take a bar of any of the above length . If while chilled they had been waxes, warm it in a bath to its working placed in the cold investment, attached temperature, bend it and hold while chill- to the same sprue and cast, the bars ing, and when it has become thoroughly would be identical, but when simply cold release it, you will find that it will the change was made of placing them apparently remain bent . Upon being in a warm investment at their upper very slightly warmed, however, it will working range, and they were then cast, straighten again . Most of the above the difference in their length was 0 .185 waxes are too brittle to allow of bending a of an inch, or a variation of 18z per straight cast bar into a hoop, but even the cent., for the warming will release the brittle ones have a large elasticity . If a elasticity, and thus the stretched bar will bar or stick of the Cleveland dental inlay shorten 0 .1, or 1/10 in., and the com- wax be warmed enough to bend into a pressed one will lengthen 0 .085, or circle until the ends touch, then chilled 85/1000 in . Each will change its length while held, and then warmed again, it by 10 per cent . or nearly so . These bars will straighten one-third of the way to so treated and cast are shown in Fig . straight ; and if again bent till the ends 4, showing A the wax before and B the meet, chilled, and then warmed, it will metal after investing and casting . straighten over 70 per cent . of the last This is a source of exceedingly large bending . S . S . White sticky-wax will, error-and it is not necessary that the 274 THE DENTAL COSMOS . wax be placed in warm water as in a study of the effect of stretching the wax warm investment, for even the warm over a form (as in a double compound summer temperature or that of a warm cavity), and the conflicting of the forces room is sufficient . For example, two of expansion and elasticity, which are bars of a commercial inlay wax were beautifully demonstrated as follows : If taken, and one was stretched and the a bar of wax be heated and thus ex- other compressed endwise, at the lower panded, and then fastened to make it working range, and chilled while held . retain that expansion (as when a warm They were then cut to the same length, wax pattern is made by the direct method namely, 4.31 in., and attached to a card in a double compound cavity-a mesio- and left in a warm part of the room over occluso-distal cavity in a molar), and night, and, were measured when cold in then cooled, the wax will be stretched Fia . 4. A B C D Two similar wax bars placed in a warm in- Two similar wax bars, showing elasticity dis- vestment and cast. A, Before heating . B, tortion when heated . c, Before heating. D, After heating. After heating . the . morning . The stretched one was owing to being held in each case, and if shortened 0 .25, or 4 in., or 6 per cent ., chilled and kept chilled will remain and the compressed one was lengthened frozen in that position, but if warmed 0 .19, or 3/16 in ., or 42 per cent . These will not expand from that position, but are shown in Fig . 4, marked c, before, will contract, owing to its elasticity, a and D, after warming. large part of the amount to which it has This part of the paper should embrace been stretched . Let us make two bars a more extended review, but space will of wax, an inch long-of, for instance, not permit of it . Anyone can make these Cleveland dental inlay wax-precisely and other simple experiments to demon- alike in cold dimension except that one strate that the elasticity of the wax may is carved directly from the cast wax stick be and is a vary large source of error, and the other from a piece of the same especially in hot weather . When wax is wax that has been worked when warm melted into a form or chilled from the and stretched as it chilled . The pattern liquid state without pressure, its elas- pieces are then attached to the same sprue ticity is negligible on warming again, gate and invested together in an invest- though its original contraction is enor- ment of plaster and silica at a tempera- mous . A comparison of patterns made ture of 128 ° F . The piece cut from the both in cast wax and in worked or unworked cast wax will expand 35/1000, stretched wax is essential here, also a or 3 .5 per cent ., and the other will, while PRICE .-THE BEHAVIOR OF GOLD IN FUSING AND CASTING . 27 5 expanding, contract endwise the amount tion would be 2 .3 per cent., which error of its elasticity, an even greater amount . goes forward in each case if the model If after burning out the wax we cast pure or pattern is placed in the investment gold into them both at the same time, material at that minimum or room tem- we shall have bars differing grea .tly perature of 67 ° F . Under these condi- in length, though the wax patterns from tions the contraction error carried for- which they were made were identical . ward by each of the waxes would be as One test of the above produced a bar follows : Bird & Moyer, 1 .2 per cent . ; of gold from the unworked cast wax Cleveland dental inlay, 1 .2 per cent . ; 27/1000, or 2 .7 per cent. longer than the Klewe, 1 .2 per cent. ; Consolidated, 1 .5 pattern, and the •other 67/1000, or 6 .7 per cent . ; Peck, 1 .4 per cent . ; S . S . per cent. shorter, from the bar of worked White black inlay, 2 .3 per cent ., and S . and stretched wax . The volume of the S . White crown sticky-wax, 1 per cent . two pieces of wax remained the same, All of these contraction errors can be but the shape of the wax did not . controlled by re-heating when investing, The only wax of the above tested waxes if the condition of the wax is not one (see Tables I and II and Fig . 3) that has of internal stress or stretch-in which not a large expansion and contraction is case the elasticity error, as just shown, that suggested by the writer for taking may double or triple the expansion error impressions for the stone model method sought, and the ultimate error is very of procedure. It also has an exception- much greater than if the wax pattern ally low proportionate elasticity, about were kept cold when investing . The er- one-tenth of that of carving waxes . The rors or changes due to elasticity of the contents of the Price impression wax are waxes is never a uniform change, but a pure- true distortion of the mass or part of it . It is probable that every member of the Wliite gum damar, 110 part s dental profession has experienced a dis- Tamaraek ( hackmatack ) , 10 tressing practical example of the contrac- Beeswax (pure), 15 tion change of beeswax when using it Paraffin, 10 for making a bite in order to articulate Stearic acid, 2 models when teeth were present in the patient's mouth . He had to either warm -melted together in the order named it to force it on to the models or carve and kept free from water . It should be the wax to let the teeth into it . Even used as cool as possible with wet fingers, if he warmed it to the temperature which and only the surface warmed soft when it had when he took the bite, it was often using . warped . It is not a carving wax, but an impres- Up to this point in our procedure, sion wax, and is used to take the impres- where we have the wax pattern invested, sions in which the hard stone models we may have accumulated an error of of the cavity are made, and the near contraction in the dimension of our cav- tooth surfaces of the same and adjoining ity pattern, if we invested at room tem- teeth, for this model method . Its total perature, of from 1 per cent . to 2 .3 per volume change from temperature is only cent., according to the inlay wax used ; from one-quarter to one-half that of the or if we heated when investing, we may various carving waxes . Its virtue con- have produced an apparent expansion sists in its not introducing much error above our starting dimension of from 1 .3 either from contraction or from elas- per cent . to 2 .3 per cent . But, while ticity. When an impression is taken with the volume change takes place regularly it at its working temperature of 98° F., with the heating, the expansion does not and is cooled to 67° F ., the contraction take place uniformly, owing to the elas- .change is only 0 .6 per cent ., whereas if ticity of the wax, which elasticity is al- the same impression were taken with S . ways present when the wax is cooled S . White black inlay wax, the contrac- under a stress . In getting the above ex- 276 THE DENTAL COSMOS . pansion of, say, 2 .3 per cent., we may FACTOR OF ERROR IN THE EXPANSION OR in some part of the wax pattern have a CONTRACTION OF INVESTMENT MATE- linear distortion change, by releasing the RIAL ON HEATING. elastic stress, of even 6 or 10 per cent . If we have taken an impression with The. next change, however, is very im- portant . It is the expansion or contrac- Price's impression wax and cooled and invested or placed the stone model ma- tion of the investment material when it terial in it at room temperature, we have is heated to burn out the wax, whereby a contraction error to carry forward of the dimension of the cavity record may 0 .6 per cent ., or if with the S . S . be changed considerably according to the procedure employed. In general, all the White crown sticky-wax a contraction error of 1 per cent . Neither of these investing compounds which contain plas- waxes are suitable for heating very much ter for a binder with silica in excess ex- when investing or when placing the pand regularly with an increase of tem- model in them . The former has a very perature up to from 800° to 1000° F ., small elasticity error, and the latter a while plaster alone expands only up to 350 ° F. Above these temperatures these large one, if warmed. In hot weather the temperature of the room is sufficient contract rapidly on heating, and all suf- to release the elastic stress and allow the fer considerable contraction in cooling as distortion to take place, though slowly, compared with either their dimension in all the inlay waxes, especially in. the when heated or before heating . The low-melting ones, which, however, have maximum expansion of the mold from least elasticity. heating, and the subsequent contraction when cold-both in fractions of 1 per cent . for the various investments-is as FACTOR OF ERROR IN THE SETTING OF follows : INVESTMENT MATERIAL . Pelton & Crane, maximum expansion 0.71 The next possible source of change in at 1000° F ., contraction on cooling to -0 .50; the dimension of our cavity record lies Pelton & Crane and one-half plaster, maximum in the setting process of the investment expansion 0.40 at 350 1 F ., contraction on material, but this is not an important cooling to 1 .10 Brophy Imperial, maximum expansion 0.48 at 900°, contraction on cooling factor, as it is small and always repre- to -1 .20 ; Sump, maximum expansion 0.40 sents an expansion . It is as follows- at 310°, contraction on cooling to -1 .50 ; in fractions of 1 per cent . : Sump and one-half plaster, maximum expan- sion 0 .35 at 350°, contraction on cooling to Pelton & Crane's inlay investing compound, 1 .40 ; Dendrolite, maximum expansion 0 .35 at 0 .18 ; Pelton & Crane and one-half plaster, 3 5 0°, contraction on cooling to -3.50 ; Dendro- 0 .1 ; Brophy Imperial, 0 .09 ; Brophy Imperial lite and one-half plaster, maximum expansion and one-half plaster, 0 .08 ; Sump, 0.09 ; Sump 0 .36 at 350°, contraction on cooling to 1 .40 ; and one-half plaster, 0 .10 ; Dendrolite, 0.09 ; Fyrite, maximum expansion 0 .38 at 350°, con- Dendrolite and one-half plaster, 0 .05 ; Fyrite, traction on cooling to -1 .20 ; Fyrite and one- 0 .10 ; Fyrite and one-half plaster, 0.05 ; half plaster, maximum expansion 0 .34 at 350° ; Peck's, 0 .07 ; Peck's and one-half plaster, contraction on cooling to -1 .50 ; Peck's, max- 0 .07 ; plaster of Paris, stiff mix, 0 .13 ; plas- imum expansion 0.70 at 1000°, contraction on ter of Paris, thin mix, 0 .10 ; I . D . L ., 0 .07 ; cooling to -0 .70 ; Peck's and one-half plaster, I . D. L. and one-half plaster, 0.8 ; Taggart's, maximum expansion 0 .32 at 400°, contraction 0 .07 ; Taggart's and one-half plaster, 0 .10 . on cooling to -1 .10 ; plaster of Paris, stiff mix, maximum expansion 0 .45 at 350°, con- traction on cooling to -1 .80 ; plaster of An error from this source or an oppor- Paris, thin mix, maximum expansion 0 .30 at tunity to correct an error from another 300°, contraction on cooling to -2 .40 ; I . source is so small as compared with the D. L., maximum expansion 0 .66 at 1000°, con- other errors or changes that we can dis- traction on cooling to -0.80 ; I . D . L . and miss the change in the setting of the one-half plaster, maximum expansion 0.35 at investment. 500°, contraction on cooling to -1 .50 ; Tag- PRICE .-THE BEHAVIOR OF GOLD IN FUSING AND CASTING . 27 7 co o p ~ L k o ~ o F ~ y a y Y 4 ~ Q ~ .\" p ul y \ ~ d o O N a C \ Y k a aa y 0 C Q y d J~ h m$ p ~i Q 0 a tl) ._,~ -5-~ h 4 ~ 4 . \ 4 \ V f E. q 0 o c E N .C ~y O +~ E bA < rti qc o O_ s7 7z W R o < O ~ Q CL L n z 0 lo U ao o `L .°. ~ a -- ,~ z Y S ~'fo 0 ~ m z au 01- - ao.t .~ c's d a O O ~ O bA q O , 1~ ~O h tl M N . . O z •qoul us jo sqlPuesnoql uI 278 THE DENTAL COSMOS. gart's, maximum expansion 0 .85 at 1000°, thereby the amount of correetion that contraction on cooling to -0 .60 ; Taggart's can be made to offset some of the un- and one-half plaster, maximum expansion 0.34 avoidable contraction . It also shows the at 300°, contraction on cooling to -1 .10 ; Price's artificial stone for models, maximum additional error that can be made by let- expansion 1 .20 at 900° ; contraction on cooling ting the investment cool again after heat- to -0 .02. ing, before casting into it . These meas- urements were mostly made in the appa- The expansion and contraction of all ratus shown in Fig . 6, which was made the above compounds at all temperatures especially for the study of temperatur e Fia . 6 . Author's expansion recorder, with muffle and pyrometer . up to 1000 .° F ., and again on cooling, expansions . The piece being studied is is recorded graphically in the chart of heated in a platinum muffle and the tem- curves of temperature in Fig . 5 . The perature recorded by the pyrometer . base line shows normal dimension, and In the selection of the temperature of the expansion in thousandths of an inch the investment when casting we can is shown in the elevation above that base control a range from increasing the size line . The temperature is shown as nor- of our cavity record by one per cent . or mal at the left, and increases in divisions o f decreasing it by two per cent .' Our toward the right . The contraction on total error to and including this step cooling is shown by the descending curves may range-first, from an accumulated to the extreme right . This chart shows contraction error of 3 or 4 per cent . to at a glance the temperature at which the a zero dimension without introducing a investments should be cast into, to secure distortion error from elasticity ; second, the maximum expansion of the mold, and to an accumulated expansion error o f PRICE .-THE BEHAVIOR OF GOLD IN FUSING AND CASTING . .2 7 9 3 per cent ., with elasticity distortion er- eighth of an inch across, and 1/91 of rors . a square inch of surface . The curves of Fig . 7 show the distance, in thousandths FACTOR OF ERROR IN THE POSSIBLE of an inch, that the plunger penetrated CHEMICAL OR PHYSICAL ACTION OF the cold blocks at the various pressures IMPRESSION WAXES UPON THE IN- at which some of the blocks collapsed . VESTMENT MATERIAL . For example, with the Pelton & Crane cold investment, 16-oz . pressure on a sur- The next possible error will arise from face 1/91 of a square inch produced an the chemical or physical action of the indentation 14/1000 of an inch deep, impression waxes upon the investment and at this pressure the cube collapsed . material . This is not a source of much Silica and plaster, four to one, broke at error, and, when it does occur, is a dis- 37 oz., and at that pressure had yielded tortion of the mold from flaking of the over 40 thousandths . Taggart's broke surface . It usually occurs only when at 37 oz ., and had only distorted or the wax is burned out after the invest- yielded 5 thousandths . The majority did ment has been allowed to dry out . A not crush at 58 oz ., and their exact yield- moist investment when heated will pro- ing at that pressure is shown on this tect the surface from the wax by the chart . The artificial stone suggested steam forcing the wax out of the surface by the writer did not indent, and was of the mold, instead of melting it into crushed only at a pressure of 16,000 lb . the surface . The error from this source per square inch . Table III shows in would be a distortion, and not a uniform detail the amount of indentation into the change in the cavity dimension . cold blocks at the pressures indicated . For demonstrating how easily the in- FACTOR OF ERROR IN THE PRESSURE OF vestment will fracture when not sup- THE MOLTEN GOLD UPON THE INVEST- ported, the following is interesting : A MENT. large investment ring is filled even with investment around a small spiral wax The next error arises from the pres- core attached to a glass tube with a flange sure of the molten gold upon the invest- to hold it in the investment, and the ment ; this is considerable in amount if wax is burned out in the ordinary way . the investment is soft owing to either The cavity is filled with mercury till it an excess of silica, or poor plaster, ' or shows in the glass tube, by applying air very thin mix, or to heating too soon pressure through a rubber tube placed after mixing and before the plaster has over the glass tube . The bursting force become strong, also to a high pressure . from the pressure of the mercury within The strength of the investing material will be sufficient to force the investment, when it is entirely cold is much greater if there are no ends in the ring, out of than when hot, which gives to readings the top and bottom of the ring, with even on cold specimens only a relative and ap- so low a pressure as 20 lb . per square proximal value . Fig . 7 shows graph- inch . In this case the conditions are not ically the effect of pressure on a cold identical or similar to those when air cubic block, one inch square, of the vari- pressure is used in casting, in which case ous investing compounds set under con- it is applied to the top of the investment ditions ideal for maximum strength . It as well as to the- metal column going indicates chiefl y their relative resistance, within . The coefficient of expansion of since the conditions for this test were all investments when heated is several not those under which we use them prac- hundred degrees less than that of the tically. The measurements were made metal rings, which latter consequently with an end comparator made by the cannot support and sustain the invest- Societe Genevieve, Switzerland . ment closely, and this readily allows of a The pressure was produced by a slight fracture and distortion . One means smooth flat round surface about one- to measure the distortion is to cast simul- 280 THE DENTAL COSMOS. C ~ ~ arti V° E o ~ \ o l Z p~ m U E~l'`~y ¢~ n~ 1 ° ie a F yoo :o ~ p~ ~ ~ ct" t tp ,a h :C . .QyY c ~ m. :a< ♦` , 0 ``\ U ♦ ` \\ - .\ " `\ `\ ♦ o ` ♦♦♦ . . ` \\ V b 1 ♦ . .\ o O v 4 0o q ~n y q ` 1 m ~ ~ ym `\ O I ` \ t~ ~ m `` ♦ Aa t ♦ b Ir4 ~ ( ti o m ,✓ m t r3 ~ ~ 1 ay ` .~ `t 1 C o~k Qm `\ 1 \ 0 \\\ 1 1 `\ 1 1 1 1 \`\ \\ t O p O W . ~ w p~ •qauj ue =o sg3Pcresnoq3 nI PRICE .-THE BEIIAVICR OF GOLD IN FUSING AND CASTING . 28 1 IaISBid % 7 ry o c v~ . . ° o .-i c.~ ro co d . • • ~. , . -_ __ -~ - _ . , N . . •sau 4i 7as p .~ " cr ~ 'Qi ua 4i ia s ~ b d a. ❑ R ialS'BTd .Q o 0 . ~ co o o m .~ a co 'S,1iB."o.3B,j ~ II ~ O 'S,~I'B2 .d~,I .:~ ~ m " ❑ ~ I! . . . . o • , • ~ o p aA •a ~ . ~ ,_ U aD "~U° 'C ~fJ aaisaid z •1'Q'I YT I . . . ._-. _- . ._ ~- .. . . . O -- . _- - ._ C do c7 ~ w ~ ~•I 'Q •I ,~ o .- . ~c o ~ . . . . ~ o y o y p ~ ~ A H N O W ~ Co IIiii1 `aagsBid I~ ~O W ~ O o 0 3 ~ o,n ,~ __ .-_ -- ^-- -- - _ . - ~ N - I'" •uznipauz`Sagsvjd . " . . . . . U F ~ I. . . . ._ I' . _ _ --- - on I " •s,~[aad %~I p ' . c~i v.~c o: ~i w ~i . ~ ~ N _ w s ~oed ! o a . . . . . ~D za~sre z - W GV M ~--I . . . . . . - - . a . . • ~ •aics6,,I o • . . ~, . . ~ . . . . W F zaisvid % . . . o • ~ • y ~ U1 •agiiospua (r L a~ ~ N • m • ~ F w 4110 apaa Q z N N M a, a ~ a ] co duzng % ,, ('aid uvs ON ) F - .. .. - . . _ _ _ . - N b V n M . ..- - G1 N r cd . ~ o ~ ~-~ Aw~ H •dmnS o ~ N _ - . . . _ ~ 3aisB[d ~ . m ° •ireFiadtnI. °. o N H . . . . -. .. . . .. . . ~~ . ~I I~ •pelsadntI . o . . o . . . . . . ai . . . N . . c7 - --._ . . - -. . - -- a ~ 'saissi d t P ~ - O - - - D anaap p uo~iad j o ~ M o O O D . . . m . . . . . . N M ~ V p .~ ' ~ b a> = ~ - o vi o ~ cV - , c~' co co p N v n ro - z N o ~ N d y~ ~ a I U ~ a N V O a~N m a I [VOL. LIII•-20] 282 THE DENTAL COSMOS . taneously a bar and a ring attached to closely to all surfaces within even sev- the same sprue gate, the wax pattern for eral thousandths or probably several hun- which must be made from wax that has dredths of an inch . been entirely relaxed to remove its elas- ticity by warming several times nearly ACTION OF THE MOLTEN GOLD ON THE to its melting-point before finally carv- INVESTMENT . ing. The bar of wax is made of a known length, and the ring is made to go over The action of the molten gold on the the base of a taper column . In each case investment is not a source of large error the change in dimension for temperature in the more recent investments which change will be the same, and can be easily contain a large percentage of silica, but determined from the data here given . In it was so in some of the early compounds fact, all the changes that affect the di- which contained fusible ingredients, as mensions will be the same for the two soda glass . In their fusing in the sur- pieces except that the distortion changes face of the mold or chamber, this was of the investment from pressure that enlarged or distorted. will affect the measurements will appear on the ends of the bar and on the inside CONTRACTION OF THE GOLD IN COOLING . of the ring . In the former the error will make it appear larger, and in the latter The universally large and fixed error that is a part of all the methods of tech- smaller . This is not a uniform change of expansion, but an uneven distortion . nique, and the one step around which The possible or probable errors from this all others hinge, is the casting of the source are so great as to cause a low pres- gold and the contraction continually at- sure to be generally used with a soft, tending its cooling to normal tempera- weak investment, and make it essential ture . This error is divided into the that a hard model or hard investment be change of dimension attending the used to cast into when a very high pres- change of the physical state from liquid sure is applied . The surface errors due to to solid (corresponding, though in a dif- beads of air or organic matter in the in- ferent direction, to the change occurring vestment should be classed as distortion when ice is formed-having an 11 per errors of the surface, and amount gener- cent. greater volume than water) and ally to a few thousandths at least . Any of the contraction from the freezing-point these sources of distortion-the compres- of the gold to normal temperature. sion of the soft investment, the checking This is the first publication, as far as and bursting of the mold, enlarging it, or the writer knows, of any data relating the surface defects of the mold under either to the fact of such change of vol- pressure-may prevent an otherwise very ume with change of state, or its nature accurate reproduction from going to and amount . While it is not an exceed- place or fitting, and will usually be er ro - ingly difficult matter to determine the neously classed as a uniform expansion, change in dimension from the frozen or even when they accompany an actual con- crystallized state down to normal tem-_ traction . The fi rst two of these forms perature, it has been an exceedingly dif- of distortion are practically eliminated ficult matter to determine quite accu- entirely from all cavity surfaces when rately the volume change attending that casting into a hard stone model or any physical change . During the winter of similar hard mold, and trouble with the 1907 and 1908 the writer determined the latter form is very greatly reduced . linear contraction change of the gold It is impracticable to try to express from its crystallizing or freezing point distortion errors as per cent . increase or to normal or room temperature (as pub- decrease in the size of the cavity record, lished in Items of Interest, May 1908), but they usually mean a large increase and found it to be 22 .5 thousandths, or at some single diameter or surface, mak- 2 .25 per cent . ; but, as stated, these de- ing it impossible for an inlay to fit terminations could only be carried to and PRICE .-THE BEHAVIOR OF GOLD IN FUSING AND CASTING . 28 3 from the temperature where the gold weight, the total reduction in volume bars still had considerable strength, and would of course be the difference between did not include any of the change of the volume of the molten column and dimension with change of state, or the the same column when cold . The con- changes occurring close to the crystal- traction of the cooling column after crys- lizing temperature . Fig. 6 shows the in- tallizing being measurable, the difference strument used . Quite continuously since would be the change due to the change that time the writer has carried on in- of state . The effect of pressure on the vestigations to determine just what oc- cooling mass would be exactly indicated curs when gold crystallizes . One of the by the relative reduction in the cross methods chiefly used to determine the section at any point, as the mass cooled total contraction of gold after freezing under its own weight, if the molten col- consisted in casting into fused quartz umn had parallel sides of known dis- chambers of known dimension, and di- tance apart . To accomplish this deter- rectly measuring the contraction . This mination, the writer had made of fused present review of the errors so far en- quartz a chamber, 25 cm . (10 in .) high, countered in the technique of casting, and 1 cm . wide and 2 mm . across . This viz, those of the wax and investments, chamber was made by placing four pieces explain fully the necessity for elimina- of fused quartz together, two narrow ting all the foregoing technique for a pieces, 3 cm . wide, being placed 1 cm . quantitative determination, because the apart, between two pieces 7 cm . wide . errors introduced would require difficult The two inner edges of the two narrow and uncertain corrections to be made . It pieces were ground very straight from becomes necessary to use as a substance and to end, approximately to within one for measuring and casting gold into, one ten-thousandth of an inch, in order to with a minimum of expansion and con- measure accurately the exact reduction traction, and the temperature ratio of in cross section of the gold column at such change must be a known quantity . all distances from the top of the column, Fused quartz has the most favorable qual- or at all pressures up to the maximum . ities of any substance available, since its The lower end of the chamber was closed dimensional change with temperature is' and the upper surfaces were ground flat about one-fortieth that of gold, and its and smooth in order to place a flat cap rate of change is known with accuracy . over the chamber to produce a column For this determination it was desired to of molten gold that precisely filled the measure the volume of the gold in the chamber . A special very large electric molten state, and again in the cold state, muffle was constructed to receive and and also at the same time, if possible, to heat the quartz vessel . It was necessary measure the effect of pressure on the lo- to have the quartz blocks made in Ger- cation of the contraction as the column many-which, together with the labor was crystallizing, the pressure at any expended in making the two straight point being equal to the weight of metal edges so accurate, made the instrument above it . very expensive . Since fused quartz has a lower expansion and contraction change DELICATE TESTS FOR ACCURATELY MEAS- with temperature than any substance that URING THE CONTRACTION OF GOLD . could be found to hold it together, it be- came impossible to hold the quartz pieces Since gold is approximately 19 .27 together at the high temperature of mol- times heavier than water, a column of ten gold under the enormous pressure molten gold a foot and a half high would of the full ten-inch column of molten have a pressure at the bottom equal to gold, which was equivalent to a column atmospheric pressure, or equal to a col- of water twenty feet high . A four-inch umn of water 30 feet high . By letting a column was the highest that could be column of molten gold of known height sustained, which gave us measurable and diameter crystallize under its own cross sections up to that pressure to de- 284 THE DENTAL COSMOS. termine the effect of pressure on the sion is approximately three times linear location of the contraction . The cham- expansion . The volume of the fused ber of fused quartz was then made in quartz chamber was determined by weigh- the form of a continuous tube with the ing the mercury which it contained, and lower end closed and the upper end making corrections for temperature and ground flat as before . This permitted buoyancy of the air, etc ., and measuring only of the determination of the entire the specific weight of the mercury used . change of volume from liquid to normal Three calibrations gave the volume of temperature, without the possibility of the fused quartz chamber at 0° C . to be measuring at the same time the effect 3 .679 cubic centimeters, and, at the melt- of pressure on the location of the con- ing-point of gold, 1064° C ., this amount traction. A special platinum wire resist- plus the cubical or volume expansion of ance muffle furnace was again made to the fused quartz cylinder to that tem- heat this one-piece quartz chamber filled perature, which, using Minchian's values with gold . A pyrometer thermo-electric for the quartz expansion is [(1 -~- 3 X couple was placed at the base of the 0 .000000449) X 1064] = 3 .686 ccm . chamber to record its temperature . To reduce the weight of the cold gold When the chamber was slightly more which filled the chamber when molten, than full of molten gold the ground-flat to volume, its specific weight was accu- cover made of artificial stone and heated rately determined by weighing in water was placed over the chamber and pressed in the balance shown in Fig . 2, and down, thus crowding off the excess as found to be 19 .267 at 0° C . The weight the temperature was held at just the of the cold gold which filled the cham- melting-point by means of the pyrom- ber when molten was determined by five eter and rheostat . This was repeated five tests, and found to be 63 .670 grains, times, and the gold was weighed with which reduced to cubic centimeters is great exactness as will be explained . This 63 .670 = 19 .267 = 3 .305 . determination of the volume change of The weighing of the gold and the mer- the gold is based on measuring the differ- cury required to be done with very great ence in the volume change of the fused accuracy, and it was done with the in- quartz and the gold, and thus determin- strument shown in Fig. 8, which is ing the volume change of the gold, that of credited with being the most sensitive the fused quartz being known. Fortu- weighing instrument on the continent . nately, this latter change has been deter- It will register, for example, the differ- mined very accurately by Mr. Howard ence in the weight of a kilogram weight Minchian of the department of physics of when lifted two inches farther from the the University of Michigan, to within earth . It is a part of the splendid equip- an error of one part in 1,500,000, by ment in physics at the Case School of the following method : A beam of mono- Applied Science . The weighing is done chromic light was passed through a fused at a distance of twelve feet from the quartz piece supported on a fused quartz balance and in a separate cabinet, the cylinder to be measured, in such a way weights being operated by a mechanism as to produce interference rings, and, extending into the double case surround- as the cylinder expanded on being heated, ing the balance . The readings are made the rings moved outward with each addi- with a telescope . It takes about two tional wave-length of distance between hours to make a single weighing, which the reflecting surfaces. In other words, can be done to witiiin one thirteen- the divisions of the ruler used for meas- thousandth part of a grain on a full uring were the waves of light themselves . load of two and one-half pounds . Mr . Minchian found the coefficient of The volume of the gold at 0° C . was linear expansion (the rate of expansion 3 .305 ccm ., and when molten at 1064° per degree) of fused quartz constant up C ., 3 .686 ccm., hence its total contrac- to 950° C . and to be 44 .9 X 10-8 = tion between these temperatures is 0 .381 0 .000000449 . Cubical or volume expan- ccm . The contraction per cubic centi- PRICE .-THE BEHAVIOR OF GOLD IN FUSING AND CASTING . 28 5 meter is 0 .381 = 3 .305 = 0 .1153, or, 16 .201 cm . or seven inches long and one- expressed in per cent ., the volume change quarter of an inch in diameter . A spe- or total contraction is 11 .53, which is cial platinum wire resistance muffle was probably much larger than any of us made for each, closely fitting to the gold, suspected . Since linear change is one- and with a thermo-electric couple at- third the volume or cubical change, the tached to the bar in the center of the total linear contraction of gold is 3 .84 muffle, and insulated from the gold as per cent . from the molten state to 0° C . it passed out . The square ends of the FIG . S . . . . ~ ~ . . - - . . . . - . . . . ~f Large precision balance . General view, showing operation from a distance . To find the part of this change that bar were covered with measured mica is due to change of state we must sub- plates to reduce radiation at that point . tract that part which takes place after The bar was heated slowly, and meas- the gold has crystallized. urements were made on the ends, at every The writer had previously determined 50° C . up to the sagging point . These this to be, as noted, 2 .25 per cent . linear measurements were made very accurately or 6 .75 per cent . volume . To verify or in an end comparator measuring to correct these measurements they were 1/100,000 in . The instrument is shown repeated with great care to eliminate all in Fig . 9 . But there was some radia- possible sources of error such as radia- tion at the ends of the bar, which error tion . Two bars of the same gold were must be eliminated. Since any two simi- made of different length, one 12 .619 cm . lar bars have the same error from radia- or about five inches long, and one-quar- tion at the exposed ends, a section in ter of an inch in diameter, and the other the center of the longer bar, left after 286 THE DENTAL COSMOS . subtracting the shorter bar, will repre- ing for end radiation, the upper the ex- sent the true expansion, since all errors pansion of the same piece after elimi- from radiation have been removed by nating end radiation, and the dotted part subtracting the shorter bar . Hence the the extension for the part of the range too two-inch section in the center of the near the melting-point for the gold to seven-inch bar left after subtracting the have strength enough to measure, so is five-inch bar will be free from radiation computed . In this chart the curve of ex- errors . These measurements are show n pansion for the fused quartz is also show n Fia. 9 . Precision end comparator, used in measuring length of gold bar . graphically for both bars in Fig . 10 . up to the same temperature, viz, the The base line represents temperature, and melting-point of the gold, and, as seen, the elevation shows expansion in hun- it is very small in comparison . dredths of a centimeter . Since the gold These more exact measurements of the has not strength within fifty degrees of expansion of pure gold up to its melt- its melting-point, that part of the curve ing-point change the second decimal of had to be computed, and is shown ex- the original determinations, making it tended in the dotted line in Fig . 11 . In 2 .20 per cent. linear instead of 2 .25 per this chart is given the expansion of a cent ., and 6 .60 per cent. volume instead bar, 1 cm. long, in thousandths of a of 6 .75 per cent . This contraction of centimeter . The base line represents the gold after crystallizing or freezing, temperature, and the elevation expan- subtracted from the total contraction, sivri . The lower curve is the expansion gives the contraction that takes place of, a 1-cm . piece from the longer or with the change of its physical state- seven-inch (16 cm .) bar, without correct- viz, expressed as volume or cubica l PRICE .-THE BEHAVIOR OF GOLD IN FUSING AND CASTING . 28 7 FIG . 10 . OBSERVED EXPANSION OF GOLD BARS . ::I I I I I I I I I I T I I 27 26 25 24 23 2•L 21 20 19 18 17 ~ 16 v ~ 15 0 14 R3 •o 13 V A 12 9 11 i t 10 9 ~+2° y 8 7 6 5 4 3 2 L I I ILI I I I I I I I 0 100 200 300 400 500 600 700 800 900 1000 1100 Degrees Centigrade . 288 THE DENTAL COSMOS: FI(I. 11 . LINEA$ EXPANSION OF PIISE GOLD, AND EXPANSION OF QUARTZ . 22 To/n/ 1-io. 0 226 at / 64"!7'/ tt 21 20 19 . . .'~ ~ Ga F' y a I . o r 18 .n O q O V Y Q . ~J7 :•~ ~ .-~ O Y d~ .y tlj Y ~ . 17 ♦ / Y N a°'c ~aug"o 16 ~j V ~ V c3 p0 . a V q F7 m V y,~a . . . . fa"CctlEi~d¢ 15 cs a a Y Vl 14 ~ oa a ~ ~ /P m 13 ~ A k an 12 ~xe M q .~ /Ce g 11 . . 0 q ~-i A y~ N eFOj ~ y Y . p S~ Y 10 Sb i7 y Ff e) O V.a ~ a ~ 9 ' .4 d d p 0 an c QC :o" ab~aw»° V 8 oo~s7~csya~i ~ . . Op047 z7 F+ CL ca>~ ~ 0 7 0 ~ w :~ o O OOy , Vl G ~ 6 ~ A w t 5 4 4 ~~d~ USSyi . O O y m ~ 3 All P4 Z3 ~ 2 O .r~ ~ 1 .. . Y Y ¢. . . pq 1 nnsi of uarh 0 100 200 300 400 500 600 700 800 900 1000 1100 Degrees Centigrade . PRICE .-THE BEHAVIOR OF GOLD IN FUSING AND CASTING . 28 9 change, 11 .53 - 6 .60 = 4 .93 per cent ., control its location . In other words, we due to change of state or latent heat of can, by .forcing in molten gold from the fusion ; or, expressed as linear contrac- sprue to take the place of the accumu- tion, 3 .84 - 2 .20 - 1 .64 per cent ., or lated contraction in the inlay, cause all linear contraction due to change of state the contraction due to change of state without change of temperature . Fig . 12 to appear in the sprue . This can only shows graphically the proportion of the be done by having the gold in the sprue contraction changes . It may be assumed molten when that in the inlay is crystal- that, wherever and whenever pure gold lized, which can best be secured by hav- is melted and cooled, these changes in ing the mass of gold in the sprue large dimension take place, and this becomes in proportion to the inlay, and by using one of the most rigidly fixed factors t o a high enough pressure to move the gol d FIG. 12 . TOTAL CONTRACTION OF GOLD . 0 .04 ^. U 0 .0 3 o b A o 0 0.02 c ~~ ®R ~°r o o T ~S o ~o 0.01 0220 ° o= 0.00 which we must adapt our technique . In in ; also by using a relatively large gate, other words, we must systematically pro- and having the investment sufficiently duce a definite error elsewhere to neu- heated so that the gold will not be quickly tralize or correct that part of this error chilled in the gate . With a high pres- that cannot be controlled . sure not only can this part of the con- traction-i.e . that due to the change of CONTROL OF THE LOCATION OF THE CON- state from liquid to solid, and amount- TRACTION OF GOLD . ing to 4 .9 per cent . of volume and 1 .64 per cent, of linear dimension-be entirely Probably no dentist who has done cast- controlled, but, if conditions are made ing has failed to see that frequently favorable as by the above suggestions, there was a hole or depression in the even a little more of the contraction than side of the casting, or even a complete the above can be controlled by pressure, separation between the .sprue and inlay . for as long as the pressure on the col- This is the result or expression of the umn of gold is greater than the strength contraction due to change of state ; it of the gold, the latter will move . Fig . is, however, an error that we can control 13 is a chart showing graphically the entirely . While we cannot prevent con- effect of pressure on gold and its alloys traction due to change of state, we can after they have passed through the change 290 THE DENTAL COSMOS . cn z E. @ U o O N+\ 0 \ a L L O L e \ : a~ m + QqN Ca to o\° to o V~j ~ o ~ W p U) \ a ° ya ~ ~F~ " "~ ; a ad a0 C~ C~ `.t U C~ N N g Q , co y) \\ \ \ 0 co 0 \\\ +\ \\ \ O \ \ \\\\ \ i \ ~ l P4 \ \ i~ \\ \ \ - \ \\ \ \ \ I~I \\ \ \ \ ~ ~ \\ O I \ \\\ 1 Q . \\\\ \+\ ~ + 0 .-~ 0 o C •slucod-2uF3lacu motaQ 3Iaquaaqg,l saaa2aQ PRICE .-THE BEHAVIOR OF GOLD IN FUSING AND CASTING . 29 1 of state and are crystallizing and cooling CONTROLLING THE GOLD BY CASTING toward zero. INTO A MODEL OF ARTIFICIAL STONE . Fortunately we have a means for cor- CONTROLLING THE GOLD BY ADDING recting a large part of this most trouble- ALUMINUM . some class of error-viz, by holding the contracting gold so rigidly that it is com- Eight ounces of positive pressure, on pelled to stretch . This is accomplished a square surface one-eighth of an inch by making the mold into which we cast square, moves pure gold, as shown by of a material so strong that the cooling this chart of curves of pressure effects, gold cannot crush it, but will itself be only 30° F . below its melting-point, and stretched . The practical material for if 0 .2 per cent . of aluminum be added casting into, that has strength enough to it, the strength of the crystal is so for this, is a hard model made of a spe- reduced that it will move 470° F . below cial silicate cement, viz, the artificial its melting- or freezing-point . Pressure stone suggested by the writer, which is of 24 oz . on the same surface will move made synthetically by fusing togethe r pure gold 200° F . below its melting- Pure silica, 20 parts point . It will be obvious that these pres- Calcium hydrate, 19 sures could only be used in practical work Aluminum oxid, 42 when casting into or against a very strong material, if it is to retain the cavity at a temperature of about 2750° F . This surfaces without distortion . Through is powdered free from iron and added the range of cooling temperature below to equal parts of a very highly vitrified the point where the pressure used will potshell, and after thorough mixing and move the congealing mass, the normal grinding together forms a very hard contraction will take place, and with pure model when mixed with phosphoric acid . gold and with the pressure that could The model becomes hard only after being be safely used with ordinary investments heated with dry heat . Great care is re- we cannot expect to do much more than quired to have the materials so balanced control the contraction due to change of chemically as to produce a model with state, though with a hard, strong invest- zero contraction on setting . It can also ment, as when casting into a stone model, be made by fusing togethe r we can control a little more . This leaves Kaolin, 3 parts by weight in general 2 .2 per cent . as a fixed con- Calcium hydrate, 1 part " traction error that cannot be prevented Aluminum oxid, 1 " " in an ordinary technique, and this error must be corrected for by introducing and treating as above. systematically an expansion error else- When inlays for double compound where sufficient to take care of it, or we cavities are cast of pure gold on such must mechanically prepare our cavity a model, the gold will be stretched and with a bevel everywhere and depend upon held . Incidentally this model method burnishing a pliable metal tightly to that has many advantages, as described in de- margin. This latter method, however, tail in Items of Interest, September 1909 . only provides a correction for the difficul- CONTROLLING THE GOLD BY CASTING ties arising from the shortening or draw- OVER THREADED IRIDIO-PLATINUM BARS . ing away of the gold from a margin of an inside dimension ; it does not relieve Another method for holding the gold those difficulties arising from the short- from contracting, or of causing it to ening of an outside dimension, as when stretch when contracting, is to cast it the metal goes over any outside surface, over iridio-platinum bars that have been like a double compound cavity or a crown threaded . This will control a large part base-where, instead of the contraction of it, if the proportion of iridio-platinum drawing the metal away from a margin to pure gold is large, otherwise the bar or surface, it draws it toward it . itself will be contracted . If the bar is 292 THE DENTAL COSMOS . not in the center of the mass, the whole The contraction after crystallization, will be warped by the uneven contrac- of 2 .2 per cent . linear or 6.6 per cent . tion . These bars answer a double pur- volume can only be corrected by-compen- pose in inlays by giving a greatly in- sation-that is, by uniformly enlarging creased strength just where most needed . the mold which is to receive it . They should be used in double compound cavities when united through a shallow RESUME OF DIMENSION CHANGES AS PRO- or narrow step in the occlusal surface, DUCED BY EACH STEP IN OUR CASTING and in the occlusal step of approxi- mal cavities . This method of preventing TECHNIQUE. the normal contraction of the gold by If we now follow through our tech- iridio-platinum bars will not, however, nique and sum up the dimension changes correct more than one-half of the nor- that can be produced by each step to re- mal contraction, depending upon the re- duce or add to this fixed contraction, lation of the masses of each, iridio-plati- we find-assuming that the contraction num bar and pure gold, and the shape due to change of state is controlled by of the casting . We can count ordinarily pressure-the following : upon one-half of 1 per cent . correction First step . In removing the pattern from this source in the occlusal step of : from the cavity we chill it, and thus re- single or double compound cavities . duce its volume from 1 .8 to 10 per The relatively exact changes of dimen- cent ., which is a linear contraction of sions that we have been reviewing as ac- 0 .6 to 2 .3 per cent . (see Table II), the companying the technique chiefly of the volume or cubical contraction being three Taggart direct method are all common to times the linear, making our contraction most inlay methods to a greater or less error, together with that of the gold of extent, and the one process which is com- 2 .2 per cent ., total 2 .8 to 4 per cent . mon to all and is the foundation of them This provides that the pattern be in- all, viz, the melting and cooling of gold, vested at its reduced temperature, at obeys the same laws in all methods . about 670 F . This is the one fixed condition to which Second step . If the wax pattern be all our technique must be adjusted, and warmed when invested, to the tempera- it may be briefly stated as follows : Gold ture at which it was when placed in when molten occupies approximately one- the cavity, this total contraction error ninth more space than when at normal can be reduced to that of the gold, of temperature, and just after changing its 2 .2 per cent ., and if heated to a higher state, or freezing, occupies approximately temperature than when it was placed in one-fifteenth more space than at normal the cavity we may get an expansion of temperature . the pattern above its original size of from The gold can be moved, when changing 1 .3 to 2 .4 per cent ., or apparently enough its state, by pressure which enables us to correct the fixed error of the gold. to determine or control the location of But we have no wax that has so little the displacement due to change of state . elasticity as to keep its form when The location of the remaining part of warmed even to the original temperature the change of dimension or contraction at which it was placed in the cavity, can only be controlled in small part by let alone permitting a higher one ; for pressure, unless a very high pressure be by heating a molded or stretched pattern used and unless a small per cent . of of any of the waxes on the market known aluminum be added to the gold to change to the writer we may introduce distor- its law of crystallization . * tion errors several times worse than the * The writer, before differentiating between error to be corrected . (See Table II the contraction due to change of state and and Fig. 4 .) We are compelled for that due to the contracting solid gold, read safety, then, until we get a better wax, pressure control as all being over the con- to invest at the lowest temperature tracting solid gold . and proceed with an accumulated error PRICE .-THE BEHAVIOR OF GOLD IN FUSING AND CASTING . 29 3 of 2 .8 to 4 .6 per cent . (the contraction between the mesial and distal pulpal of both the wax and the gold), accord- walls of a double compound inlay . In ing to the pattern wax used . result, this error is the contraction of the Fourth step. We may ignore the solid gold . Its correction comes in the change in dimension of the investment next step . in the process of setting, and pass to Twel f th step . The holding of the gold, that due to heating and cooling the in- causing it to stretch, is done over a hard vestment. model or over iridio-platinum bars in its Fi f th step . (See Fig . 5 .) This step mass, which will permit us to control of heating the investment will give us nearly all of the error due to shortening a choice, according to the technique em- of the outside dimension of the mass of ployed, of an expansion of about 1 per the gold, if it is not too large in propor- cent . or anything less, to a contraction tion to the mass of the artificial stone or of 2 per cent ., if, after heating a thin other hard model inside it . But this will mix with an excess of plaster, we let it only apply to the gold surrounding a cool off and become cold before casting . core, as the mesio-distal diameter of the If we cast at the best temperature for mass of gold between a mesial and distal maximum expansion (see Fig . 5) our filling in a double compound cavity total error will at this point represent ~where these cavities are united across the a contraction of from 0 .8 to 3 .6 or even occlusal surface, or where the gold sur- to 6 .6, if the investment used has con- rounds a mass, as a crown base or a ring . tracted instead of expanding . The writer has a taper column of brass We will pass the sixth step, viz, the on which very many rings of wax have effect of the wax on the investing mate- been made and cast in gold by different rial, as it is not an important source of operators and methods, and the only error. rings the writer has ever seen that were Seventh step . The pressure of the actually as large as the mandrel on which gold in the investment material will al- they were formed were those cast over ways produce a serious distortion error artificial stone ; and by using a grade of if the investment material is very weak stone that expands on setting they would aii~~ ~,e pressure high . It will appear pass over the base of the mandrel or in the form of distortions, and not as taper column easily . uniform expansion . It is overcome en- tirely on the cavity surfaces of the inlay We have, then, as the best results avail- by ca,4ting into a hard model in the able by the present materials and present investn:Ient . technique a final contraction error for Eighth step . The action of the gold inside dimensions of, at best, 0 .8 per on the investment we can pass, as being cent ., and from this up to 3 or even but slight . 6 per cent ., according to the materials Ninth step . The change of dimension and technique used-which will preven t due to change of state will be corrected ,-a gold restoration from going to place for by pressure ; it would not appear as over an outside dimension . In such a a uniform contraction, but as a fault in condition, if the gold can be held it can be the side of the inlay . stretched, thus correcting this most seri- Tenth step . The contraction of the ous error . The surface errors and the solidified gold has already been included distortion errors may be enormous ; they as a fixed contraction of 2 .2 per cent . may be mistaken for expansion, and are Eleventh step . The distortion of the generally sufficient to prevent an other- mold of the cooling gold includes all con- wise perfect reproduction, if we had it, ditions under which the gold surrounds from going to place ; hence the making of some investment which is not strong a joint within 1/1000 in . close at every enough to hold its shape as the gold con- point around cavities by casting a per- tracts, permitting distortions such as the fect inlay is at present impossible . The crushing of the core in a crown base or uncontrollable contraction of the gold .. . . r. ~. s ` ~ . . . . ~, ..!-. 294 THE p .ENTAL COSMOS. also makes this a physical impossib itty . and principles that have not bee n studie d as yet. in connection with the other and alder" sciences . It is not `the writer's privilege t 'say FINAL CONTROL IN THE BEVELING OF ' :•Wha t the lm ount of errOr, is i~ the Gh}- THE CAVITY MARGINS AND BIIRNj~H ~ ;r e of his fellow praCtltlIYIl8T3,'1)t tL~ ING OF THE INLAY. as both from the techni que used and Hence We must use a mechanical marrs the results shown that it is often ver y for closing within 1/10,000 inch e ry *.~ fl~(.~e indeed, an d very few in th e part of the margin of an inlay, andis profession are regularly ly producing gol d the writer believes can be accompl ik , ed inlays that do not show at some poi nt with even all our at present uncontrqlled a trace of a (36men t line, which high ideal errors, involved in even the best teeh- in the majority of cavities it is toda y nique, by preparing all cavities with bevel possible to attain . This fact, viz, our margins and providing a chisel-shaped imperfect results, and the ignorance re- gardmg the principles and physical prop margin of gold to cover every bord er' of - . every cavity, which margins must ~ro of. erties of the materials involved, which a pliable metal to be burnished and ignorance causes these imperfect results , ished to the tooth while the cement~a ; have induced the writer to make this ex - soft . This means only pure gold fo r haustive study . He believes that the de - margin s, and added strength should be, mand of the profession of tomorrow wil l gotten wherever required by casing in be that every dentist assuming to ren - iridio-platinum, preferably in the forrn ti ,der the best service must make himsel f of threaded bars . familiar with the physical properties and the laws governing the behavior of the materials which determine the perfec 'o n ESTABLISHMENT OF RESEARCH LABORA- of his service . In other words, TORIES ADVOCATED. know the fixed conditions, an himself and the variable' cond ' The art of casting will be greatly bene- those fi xed conditions, to pro fited by the perfecting of pattern and highest possible perfection . F pression waxes free from elasticity er rQ'p ple, if any dentist will take t h but with good expansion and wide wor V • ,i,mpression wax that he uses a ing range, and by an investing mediurp : 1igs . 1, 2, and 3, and Table I T that will expand on heating 2 or 3 per,. -faithfu lly the behavior of tha t cent. linear, and also be hard and strong wax, and note how he shal to permit of high pressures . produce the least amount of The profession should establish re- then turn to the investmen s s o search laboratories equipped and main, ~ * ~;aphical.ly in Fig. 5, and' note at wha t tained for continually following up an A,_,. temperature the investment which h e perfecting these fundamental requir e, .uses should be cast in order to produce ments for our professional services, a s; . Jhe maximum expansion, he will pr 4h - the rapid march of dental progress is ~bly, in a few minutes, see at ' which ate h constantly presenting new problems ancI lie can reduce his present casting error s methods that are based upon material s. 4everal fold . z-. r'q